How is surface tracking resistance measured?

Surface tracking resistance is measured by subjecting the surface of the insulator to voltage and to controlled wet contamination, and observing whether conductive paths form or whether the material fails under a defined criterion.

How the test reproduces reality

In service, tracking appears when dirt and moisture form a conductive film on an energized insulator. The test reproduces that situation on a small scale and in accelerated form: a clean, flat surface, two electrodes, a voltage and an electrolyte supplied in a controlled way.

What is controlled

  • Electrodes: material, shape and spacing, and the force with which they rest on the specimen.
  • Contaminant: composition and conductivity of the solution, and how often it is applied.
  • Voltage: level and waveform.
  • Specimen: thickness and surface condition, which must be clean and undamaged.

Failure criteria

Failure is deemed to occur when the leakage current exceeds a threshold for a defined time, or when the material ignites or is punctured. In tests at constant voltage over a period of time, the check is whether the material lasts that time without failure. In variable-voltage tests, the aim is to find the maximum level it withstands.

Test families

There are drop methods on a flat surface, which give the comparative index, and inclined-plane methods with a continuous flow of contaminant, which are more severe and suited to outdoor materials or demanding applications. The results of one do not carry over to the other. The details are in the corresponding standards, and the current edition should be consulted.

What the engineer observes

During the test, small sparks, a dry band, carbonization and, if the material is susceptible, a visible carbonized path are seen. Some materials do not form carbon but suffer erosion, so material is lost without a conductive path forming; these are reported as erosion.

How to interpret the result

There is natural scatter between specimens, which is why several are tested and the value is reported according to the method. Do not forget that the color and fillers of the compound change its behavior: the test is valid for the formulation tested, not for the whole polymer family.