24/7 emergencies 814 777 6921812 230 6079WhatsApp 811 786 0768
Electrónica MonterreyElectrónica MonterreyLaboratorios Creativeit Talk to an engineer
Menu

How is the permittivity of a powder measured?

The permittivity of a powder is measured by compacting it or containing it in a sample holder of known geometry, measuring the effective permittivity of the mixture of particles and air, and correcting it with a mixing model to estimate that of the solid material.

The problem of air

A powder is not a continuous solid: it is a mixture of particles and the air in the spaces between them. The permittivity measured is the effective permittivity of that mixture, which is lower than that of the compact material because air has a permittivity close to unity. The result therefore depends on how much air is present, that is, on the density at which the powder is packed.

How the measurement is made

  • Sample holder: a cell of known volume, such as a section of coaxial line or waveguide, a capillary inside a resonant cavity or a plate cell, depending on the frequency.
  • Reproducible filling: it is always filled and compacted in the same way, and weighed to determine the bulk density.
  • Measurement: the effective permittivity is obtained with the method appropriate to the frequency band.

From the effective value to that of the material

To estimate the permittivity of the solid, mixing models are used, which relate the effective permittivity to the volume fraction of the particles and of the air. There are several, such as the Maxwell Garnett and Bruggeman forms or logarithmic relations of the Lichtenecker type, and none is universal: their validity depends on the shape and concentration of the particles. The soundest approach is to measure at several packing densities and extrapolate toward the compact solid, checking that the results are consistent with one another.

Common sources of error

  1. Heterogeneous packing, with gaps or density gradients.
  2. Moisture adsorbed on the surface of the particles, which raises the apparent value.
  3. Particle size comparable to the wavelength, which causes scattering not accounted for in the model.
  4. A poorly fitted sample holder wall, which leaves a layer of air.

What the engineer sees

If the effective permittivity rises clearly when the powder is compacted, you are seeing the reduction of air, not a change in the material. Always report the bulk density or the volume fraction along with the value.

When another approach is better

If what matters is the solid material, it is preferable to sinter or press a dense pellet and measure it as a solid. If what matters is the powder as it will be used, the effective value with its density is the useful figure.

We do real tests, on video! Watch them on our YouTube channel →

Do you have a problem nobody has been able to measure?

Talk directly to the engineer in charge, with no middlemen.

Talk to an engineer